Talking about how to reduce the wave soldering tin oxide

文章出處: 發布時間: 2011年5月22日 人氣 5931

wave soldering process is widely used two-wave, the first peak is the cylindrical wave (mainly used for welding secret plot of the SMD components, easy to exhaust air, reducing the weld), the width of the wave surface more narrow. The second peak for the flat wave, crest flat, stable, like a mirror, the flow rate to slow. There are always new waves on the surface of liquid tin and oxygen exposure, tin oxide in liquid slag is formed under rapid flow of material, it is very different from the static oxidation, the oxidation of dynamic slag formed when there are three forms.
(1) the surface oxide film. Tin tin furnace liquid material at high temperatures, exposure to oxygen in contact with each surface and oxidized. This is the main component of the surface oxide film SnO. As long as the liquid state is not destroyed, it can play a role in the absence of air to protect the inner solder
not continue to oxidation.
(2) black powder. Produced in liquid junction with the mechanical shaft, causing rotation around the axis of the vortex surface, oxide-axis movement by the friction with the ball. While rubbing the surface of the particle temperature, and increased oxidation.
(3) oxidation residue. Tin stove generator improper design formed violent rolling surface, oxygen in the air is continuously inhaled tin material inside. Because a limited number of inhaled oxygen, oxidation is not sufficient to produce large amounts of silver within the sand-like (or rubbish-like) oxidation residue. The content of the slag in the oxidation accounts for the main ingredient, and some can reach more than 90%.
result of the above oxide slag formation and composition, to reduce the oxidation residue from the following aspects:
1. Tin surface level is not too low: level too low to increase the crest of the gap, increasing the area of ??contact with air and liquid tin tin bath down the impact of surface intensified roll
2. Slag too frequent: tin-tin oxide surface with the absence of air to do with tin oxide is inversely proportional to the speed and time, but frequently exacerbated slag tin oxide.
3. Crest play too: an increase of flow rate and the impact of tin, to increase the amount of oxygen combined with tin.
4. Tin stove vents designed to change: my company after long-term efforts and communication with customers, broke and now the equipment factory tin stove design ideas, the installation of diversion tank, oxidation sets and jet width adjusting mechanism, greatly reducing the a tin of liquidity, measured by the oxidation of slag at the customer's weight, every 8 hours not more than 1.2KG (200 width of the PCB). To save customers a lot of resources.

主站蜘蛛池模板: 久久九九精品国产免费看小说| www夜片内射视频日韩精品成人| 国产精品vr专区| 人妻少妇精品视频一区二区三区 | 欧美成人www免费全部网站| 国产一区二区三区不卡在线观看 | 国产区在线观看成人精品| 久久青草精品欧美日韩精品 | 一区二区三区四区在线 | 网站| 亚洲综合一区无码精品| 国产亚洲精品久久久闺蜜| 久久99精品国产免费观观| 无码成人片在线播放| 亚洲女同精品一区二区| 人妻大战黑人白浆狂泄| 免费大黄美女片免费网站| 校花高潮抽搐冒白浆视频| 国产成人麻豆精品午夜福利在线| 亚洲夂夂婷婷色拍ww47| 国产开嫩苞在线播放视频| 成 人影片 aⅴ毛片免费观看| 日本高清免费毛片久久| 台湾无码av一区二区三区| 日本欧美视频在线观看三区| 国产亚洲精品久久yy5099| 超清无码熟妇人妻av在线电影| 亚洲成亚洲成网| 男人扒女人添高潮视频| 国产剧情麻豆女教师在线观看| 国产精品毛片av999999| 亚洲一区中文字幕日产乱码| 色偷偷av老熟女| 亚洲 欧美 日韩 综合aⅴ电影| 国产精品三级一区二区| 精品国产福利一区二区| 精品无码久久久久国产手机版| 少妇无码av无码专区线| 手机在线看永久av片免费| 精品一区二区三区免费视频| 永久免费无码国产| 久久精品国产99精品国产2021|